Saturated Polyester
Elapol® is our worldwide brand of saturated polyester polyols for flexible and rigid PU foams, casting elastomers and TPU, polyurethane adhesives and coatings, and polyurethane systems for footwear.
Branched Saturated Polyesters manufactured with synthetic acids and glycols.
Used in flexible foam production, mainly for textile and automotive industry
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 70213 | Aromatic / Aliphatic | MPG | Highly branched | Liquid | 197 - 213 | ≤ 4 | 7000 - 10000 (35°C) | ≤ 0,10 | ≤ 150 |
| FIELD OF USEMainly used blended (up to 50%) with other polyester polyols, e.g. Elapol 7025 B, to obtain low scorching semi-rigid foams. | |||||||||
| 7025 B | Aliphatic | DEG | Branched | Liquid | 59 - 63 | 0,9 - 1,5 | 8800 - 9800 (35°C) | ≤ 0,10 | ≤ 150 |
| FIELD OF USEUsed in flexible slabstock foam production, mainly for textile industry applications (e.g. flame lamination). | |||||||||
| 7025 F | Aliphatic | DEG | Branched | Liquid | 57 - 63 | 0,8 - 1,5 | 18000 - 21600 (25°C) | ≤ 0,10 | ≤ 150 |
| FIELD OF USEUsed in flexible slabstock foam production, mainly in the automotive industry. | |||||||||
Aromatic and hybrid polyester polyols to produce rigid foams with high fire resistance,
high rigidity and improved mechanical properties.
| PU THERMAL INSULATION | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT |
|---|---|---|---|---|---|---|---|---|
| ELAPOL | mg KOH/g | mg KOH/g | mPa·s | % | ||||
| 80250 | Aromatic / Aliphatic | DEG | Linear | Liquid | 230 - 270 | ≤ 1,5 | 3000 - 4500 (25°C) | ≤ 0,15 |
| FIELD OF USENot modified polyester polyol with reduced viscosity and moderate reactivity without flame retardant. Can be used as a co-polyol. | ||||||||
| 80315 B | Aromatic | DEG | Linear | Liquid | 300 - 330 | ≤ 2.0 - 3.0 | 2000 - 3000 (25°C) | ≤ 0,15 |
| FIELD OF USEStandard polyester polyol for general purpose in rigid foams applications: lamination, spray or as a co-polyol in foam systems. | ||||||||
| 81190 | Aromatic / Aliphatic | DEG | Linear | Liquid | 180 - 200 | ≤ 1 | 3000 - 8000 (25°C) | ≤ 0,10 |
| FIELD OF USEPolyol with a low hydroxyl number for MDI savings. With reduced viscosity and slightly modified for blowing agent emulsification. Contains flame retardant. | ||||||||
| 81250 | Aromatic / Aliphatic | DEG | Linear | Liquid | 230 - 250 | 1,9 - 2,5 | 3000 - 4500 (25°C) | ≤ 0,15 |
| FIELD OF USESlightly modified polyester polyol for general purpose in rigid foams applications: lamination, spray or as a co-polyol in foam systems with increased acid value for reduced reactivity. | ||||||||
| 83240 A | Aromatic | DEG | Linear | Liquid | 230 - 250 | 1,9 - 2,5 | 3000 - 4500 (25°C) | ≤ 0,15 |
| FIELD OF USEUsed in metal and flex faced rigid PIR foams for continuous production. Contains flame retardant. Very good emulsion stability with blowing agent. Good fire and mechanicals. It works well with different pentane isomers. | ||||||||
| 81241 | Aromatic | DEG | Linear | Liquid | 230 - 250 | 0,6 - 1,5 | 2000 - 4500 (25°C) | ≤ 0,15 |
| FIELD OF USEUsed mainly in High Speed Flex Faced PIR boards production. Does not contain flame retardant. Excellent compatibility with blowing agent, very fast emulsification and low foams lambda | ||||||||
| 83242 | Aromatic | DEG | Linear | Liquid | 230 - 250 | 1,8 - 2,5 | 3000 - 6000 (25°C) | ≤ 0,15 |
| FIELD OF USEUsed in metal and flex faced rigid PIR foams continuous production. Reduced viscosity for easy processing, no flame retardant. Improved compatibility with the blowing agent and emulsification speed. | ||||||||
| 81195 H | Aromatic | DEG | Linear | Liquid | 190 - 200 | 1,3 - 1.7 | 3000 - 5000 (25°C) | ≤ 0,15 |
| FIELD OF USEUsed mainly in flex faced PIR boards on high speed lines, optimized for good quality and thermal performance. Low hydroxyl number for MDI savings | ||||||||
| 87251 | Aromatic | DEG | Linear | Liquid | 230 - 270 | 1,0 - 1,5 | 6000 - 8500 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol with approx. 40% of r-PET optimised for good processing and fire performance, low post expansion and thermal performance of the produced PIR foams. Used mainly for flex faced boards production. | ||||||||
| 87190 | Aromatic / Aliphatic | DEG | Linear | Liquid | 170 - 190 | ≤ 2.0 | 3000 - 6000 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol with approx. 20% of r-PET with low hydroxyl number for MDI savings. | ||||||||
| 85251 | Aromatic / Aliphatic | DEG | Linear | Liquid | 240 - 260 | ≤ 3.0 | 3000 - 4500 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol for metal panels and flex faced boards designed for improved fire performance. Can be used as co-polyol. | ||||||||
| 85221 | Aromatic / Aliphatic | DEG | Linear | High Viscosity Liquid | 210 - 230 | ≤ 2.0 | 10000 - 13000 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol is designed to greatly boost fire performance due to its high aromatic content. It can be used as sole polyol but also as co-polyol in PIR formulations. | ||||||||
| 85252 | Aromatic / Aliphatic | DEG | Linear | Liquid | 250−265 | 1,6−2,6 | 3500−6000 (25°C) | ≤ 0,15 |
| FIELD OF USEUsed in metal and flex faced rigid PIR foams with improved fire performance. Does not contain flame retardant. Slightly improved pentane emulsification | ||||||||
| 81180 | Aromatic | DEG | Linear | Liquid | 170 - 190 | 0,5 - 1,0 | 3000 - 8000 (25°C) | ≤ 0,15 |
| FIELD OF USELow-hydroxy polyol is designed for MDI savings. Low acid value and improved blowing agent emulsification enable high production speed with good quality. Used mainly in flex-faced insulated boards production. | ||||||||
| 83246 | Aromatic / Aliphatic | DEG | Linear | Liquid | 200 - 215 | 1,8 - 2,4 | 7800 - 8500 (25°C) | ≤ 0,15 |
| FIELD OF USELow-hydroxy polyol is designed for MDI savings. Moderate acid value and improved blowing agent emulsification enable high production speed with good quality. Used mainly in flex-faced insulated boards production | ||||||||
| 83408 | Aromatic | DEG | Linear | Liquid | 250 - 270 | 2,1 - 2,7 | 4500 - 6500 (25°C) | ≤ 0,15 |
| FIELD OF USEUsed in metal and flex faced rigid PIR foams for continuous production. Very good emulsion stability with blowing agent. Good fire and mechanicals. It works well with different pentane isomers. No flame retardant. | ||||||||
| 85190 | Aromatic / Aliphatic | DEG | Linear | Liquid | 185 - 200 | 0,9 - 1,9 | 3500 - 5000 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol for metal panels and flex faced boards designed for improved fire performance. Can be used as co-polyol. Contains TCPP. | ||||||||
| OCF | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT |
|---|---|---|---|---|---|---|---|---|
| ELAPOL | mg KOH/g | mg KOH/g | mPa·s | % | ||||
| 83201 | Aromatic / Aliphatic | Secondary OH | Linear | Liquid | 180 - 200 | 1.4 - 1.8 | 2000 - 4000 (25°C) | ≤ 0,10 |
| FIELD OF USEIs an aliphatic - aromatic, polyester polyol with superior purity manufactured from virgin raw materials. Small addition of secondary hydroxyl groups gives low reactivity for extended shelf life of the final product. | ||||||||
| 81152 | Aromatic | Secondary OH | Linear | Liquid | 140 - 160 | ≤ 2.0 | 1500 - 2500 (25°C) | ≤ 0,10 |
| FIELD OF USEIs an aromatic, polyester polyol with superior purity manufactured from virgin raw materials. Low reactivity from secondary hydroxyl groups for extended shelf life of the final product. | ||||||||
| SPRAY FOAMS | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT |
|---|---|---|---|---|---|---|---|---|
| ELAPOL | mg KOH/g | mg KOH/g | mPa·s | % | ||||
| 87241 | Aromatic | DEG | Linear | Liquid | 230 - 250 | ≤ 1.0 | 1500 - 2500 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol with approx. 30% of pure r-PET and low Acid Value for fast reactivity of spray foams can be used as a co-polyol in continuous lamination of rigid foams. | ||||||||
| 83250 | Aromatic / Aliphatic | DEG | Linear | Liquid | 230 - 270 | ≤ 1.5 | 1400 - 1800 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol with moderate reactivity and modified backbone for low viscosity for easy handling and good processability in spray foams | ||||||||
| 85250 | Aromatic | DEG | Linear | Liquid | 240 - 260 | ≤ 3 | 3000 - 4500 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol is designed for improved fire performance in spray foams, higher Acid Value gives a wider operating window. | ||||||||
| 87291 | Aromatic | DEG | Linear | Liquid | 280 - 300 | ≤ 3.0 | 5500 - 8000 (25°C) | ≤ 0,15 |
| FIELD OF USEPolyol with approx. 30% of r-PET and moderate Acid Value for fast reactivity of spray foams can be used as a co-polyol in continuous lamination of rigid foams. Polyol is designed for improved fire performance. | ||||||||
Saturated Polyesters manufactured with synthetic acid and glycols. Gives good Hydrolysis resistance and good mechanical properties.
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 5520 A | Aliphatic | 1,4-BDO, MEG | Linear | Waxy | 54 - 58 | ≤ 0,7 | 4700 - 5200 (35°C) | ≤ 0,1 | ≤ 50 |
| 5520 C | Aliphatic | 1,4-BDO, MEG | Linear | Waxy | 54 - 58 | ≤ 0,5 | 4000 - 5100 (35°C) | ≤ 0,1 | ≤ 100 |
| 5420 A | Aliphatic | 1,4-BDO, MEG | Linear | Waxy | 54 - 58 | ≤ 0,4 | 4700 - 5200 (35°C) | ≤ 0,1 | ≤ 50 |
| 5530 A | Aliphatic | 1,4-BDO, MEG | Linear | Solid | 35 - 38 | ≤ 0,7 | 10.000 - 11.000 (35°C) | ≤ 0,1 | ≤ 100 |
| FIELD OF USEVery good physical and mechanical properties. Can be used to produce cast elastomers and TPU (thermoplastic polyurethane elastomers). | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 3030 A | Aliphatic | MEG | Linear | Solid | 37 - 40 | ≤ 0,7 | 2300 - 2600 (60°C) | ≤ 0,1 | ≤ 100 |
| 3020 A | Aliphatic | MEG | Linear | Solid | 54 - 58 | ≤ 0,7 | 450−600 (75°C) | ≤ 0,1 | ≤ 100 |
| 3010 A | Aliphatic | MEG | Linear | Solid | 108 - 116 | ≤ 0,7 | 450 - 650 (50°C) | ≤ 0,08 | ≤ 100 |
| FIELD OF USEGood general properties. These products combine competitive prices and good performances. They can be used with NDI or MDI to produce cast elastomers or with MDI in the production of TPU. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 5030 A | Aliphatic | 1,4-BDO | Linear | Solid | 37 - 40 | ≤ 0,5 | 2500 - 4000 (60°C) | ≤ 0,05 | ≤ 50 |
| 5020 A | Aliphatic | 1,4-BDO | Linear | Solid | 54 - 58 | ≤ 0,5 | 1300 - 1500 (60°C) | ≤ 0,1 | ≤ 40 |
| 5010 A | Aliphatic | 1,4-BDO | Linear | Solid | 114 - 122 | ≤ 0,3 | 200 - 400 (60°C) | ≤ 0,05 | ≤ 30 |
| FIELD OF USEVery good physical and mechanical properties. Good hydrolysis resistance. They can be used to produce cast elastomers and TPU. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 6030 A | Aliphatic | 1,6-hexanediol | Linear | Solid | 35 - 49 | ≤ 0,7 | 2800 - 3100 (60°C) | ≤ 0,1 | ≤ 50 |
| 6020 A | Aliphatic | 1,6-hexanediol | Linear | Solid | 54 - 58 | ≤ 0,5 | 1100 - 1300 (60°C) | ≤ 0,1 | ≤ 100 |
| 6010 B | Aliphatic | 1,6-hexanediol | Linear | Solid | 108 - 118 | ≤ 1,0 | 300 - 500 (50°C) | ≤ 0,1 | ≤ 100 |
| FIELD OF USEExcellent physical and mechanical properties, especially at low temperature. Good hydrolysis resistance. Mainly used in the production of TPU. | |||||||||
Saturated Polyesters manufactured with synthetic acid and glycols. Excellent physical and mechanical properties and flexing resistance.
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 2020 B | Aliphatic | MEG, DEG | Linear | Waxy | 54 - 58 | ≤ 0,5 | 4200 - 4700 (35°C) | ≤ 0,1 | ≤ 150 |
| FIELD OF USEMainly used in the production of PU in solution for coating and direct coating. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 5520 A | Aliphatic | 1,4-BDO, MEG | Linear | Waxy | 54 - 58 | ≤ 0,5 | 4000 - 5100 (35°C) | ≤ 0,1 | ≤ 100 |
| 5420 A | Aliphatic | 1,4-BDO, MEG | Linear | Waxy | 54 - 58 | ≤ 0,4 | 4700 - 5200 (35°C) | ≤ 0,1 | ≤ 50 |
| 5520 C | Aliphatic | 1,4-BDO, MEG | Linear | Waxy | 54 - 58 | ≤ 0,5 | 3000 - 5000 (40°C) | ≤ 0,03 | ≤ 50 |
| 5508 A | Aliphatic | 1,4-BDO, MEG | Linear | Waxy | 136 - 140 | ≤ 0,5 | 1600 - 1800 (25°C) | ≤ 0,1 | ≤ 60 |
| FIELD OF USEMainly used in the production of PU in solution for coating and coagulation. Very good physical and mechanical properties. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 5030 A | Aliphatic | 1,4-BDO | Linear | Solid | 37 - 40 | ≤ 0,5 | 2500 - 4000 (60°C) | ≤ 0,05 | ≤ 50 |
| 5020 A | Aliphatic | 1,4-BDO | Linear | Solid | 54 - 58 | ≤ 0,5 | 1300 - 1500 (60°C) | ≤ 0,1 | ≤ 40 |
| 5010 A | Aliphatic | 1,4-BDO | Linear | Solid | 114 - 122 | ≤ 0,3 | 200 - 400 (60°C) | ≤ 0,05 | ≤ 30 |
| FIELD OF USEUsed in the production of PU in solution and in granules. Excellent physical and mechanical properties and flexing resistance even at low temperature. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 9020 A | Aliphatic | 1,4-BDO, NPG | Linear | Liquid | 54 - 58 | ≤ 1 | 8200 - 9800 (35°C) | ≤ 0,1 | ≤ 100 |
| 9010 A | Aliphatic | 1,4-BDO, NPG | Linear | Liquid | 108 - 116 | ≤ 1 | 1800 - 2600 (35°C) | ≤ 0,1 | ≤ 100 |
| FIELD OF USEUsed in the production of coating PU resins and in the processes of coagulation. Excellent physical and mechanical properties with good resistance to hydrolysis. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 10030 A | Aromatic/ Aliphatic | 1,6-hexanediol | Linear | Solid | 33 - 37 | ≤ 0,7 | 5100 - 7000 (70°C) | ≤ 0,08 | ≤ 200 |
| 10020 A | Aromatic/ Aliphatic | 1,6-hexanediol | Linear | Solid | 54 - 58 | ≤ 0,8 | 900 - 1300 (75°C) | ≤ 0,08 | ≤ 150 |
| FIELD OF USEUsed in the production of water-based PU dispersions for leather finishing. Excellent physical and mechanical properties; high hydrolysis resistance. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 6510 B | Aliphatic | 1,6-hexanediol, NPG | Linear | Solid | 117 - 123 | < 0,6 | 250 - 300 (60°C) | < 0,1 | < 100 |
| 6520 B | Aliphatic | 1,6-hexanediol, NPG | Linear | Solid | 54 - 58 | < 0,7 | 5000 - 5800 (35°C) | < 0,1 | < 100 |
| FIELD OF USEExcellent hydrolysis resistance and good flexibility in a wide temperature range. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 4028 A | Aliphatic | DEG | Linear | Liquid | 38 - 42 | ≤ 0,8 | 7000 - 8000 (35°C) | ≤ 0,08 | ≤ 100 |
| 4010 A | Aliphatic | DEG | Linear | Liquid | 108 - 116 | ≤ 1 | 900 - 1150 (35°C) | ≤ 0,1 | ≤ 100 |
| 4004 A | Aliphatic | DEG | Linear | Liquid | 271 - 289 | ≤ 0,8 | 280 - 380 (25°C) | ≤ 0,08 | ≤ 100 |
| FIELD OF USEMainly used in the production of PU in solution for coating. Excellent elastomeric properties and average general features. | |||||||||
Saturated Polyesters manufactured with synthetic acid and glycols used in the production of Adhesives for Footwear, Flexible Packaging and Hot Melt.
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 5030 A | Aliphatic | 1,4-BDO | Linear | Solid | 37 - 40 | ≤ 0,5 | 2500 - 4000 (60°C) | ≤ 0,05 | ≤ 50 |
| 5020 A | Aliphatic | 1,4-BDO | Linear | Solid | 54 - 58 | ≤ 0,5 | 1300 - 1500 (60°C) | ≤ 0,1 | ≤ 40 |
| 5010 A | Aliphatic | 1,4-BDO | Linear | Solid | 114 - 122 | ≤ 0,3 | 200 - 400 (60°C) | ≤ 0,05 | ≤ 30 |
| FIELD OF USEGood physical and mechanical properties. Good hydrolysis resistance. Used in the production of granules and solvent based polyurethane adhesives. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 6030 A | Aliphatic | 1,6-hexanediol | Linear | Solid | 36 - 40 | < 0,5 | 1600−1800 (70°C) | < 0,1 | < 100 |
| 6020 A | Aliphatic | 1,6-hexanediol | Linear | Solid | 54 - 58 | < 0,5 | 560 - 760 (70°C) | ≤ 0,1 | < 100 |
| 6010 B | Aliphatic | 1,6-hexanediol | Linear | Solid | 108 - 118 | < 1 | 300 - 500 (50°C) | ≤ 0,1 | < 100 |
| FIELD OF USEExcellent physical and mechanical properties, especially at low temperature. High hydrolysis resistance. Used in the production of granules and solvent based polyurethane adhesives. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 11110 B | Aromatic/ Aliphatic | 1,4-BDO | Linear | Liquid | 110−114 | < 1 | 7000 - 7800 (25°C) | < 0,1 | < 150 |
| 11117 B | Aromatic/ Aliphatic | 1,4-BDO | Linear | Liquid | 62−66 | < 0,8 | 5400 - 6200 (50°C) | < 0,08 | < 100 |
| 11108 B | Aromatic/ Aliphatic | 1,4-BDO | Linear | Liquid | 133−143 | < 1 | 1700 - 2200 (25°C) | < 0,1 | < 100 |
| FIELD OF USEGood flexibility in a wide temperature range. Used for one- and two-component adhesives, usually in ethyl acetate solution. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 6520 B | Aliphatic | 1,6-hexanediol, NPG | Linear | Liquid | 54 - 58 | ≤ 0,7 | 5000 - 5800 (35°C) | ≤ 0,1 | ≤ 100 |
| 6510 B | Aliphatic | 1,6-hexanediol, NPG | Linear | Liquid | 117 - 123 | ≤ 0,6 | 250 - 300 (60°C) | ≤ 0,1 | ≤ 100 |
| FIELD OF USEExcellent hydrolysis resistance and good flexibility in a wide temperature range. Used for one- and two-component adhesives, usually in ethyl acetate solution. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 4028 A | Aliphatic | DEG | Linear | Liquid | 38 - 42 | ≤ 0,8 | 7000 - 8000 (35°C) | ≤ 0,08 | ≤ 100 |
| 4010 A | Aliphatic | DEG | Linear | Liquid | 108 - 116 | ≤ 1 | 900 - 1150 (35°C) | ≤ 0,1 | ≤ 100 |
| FIELD OF USEGood flexibility in a wide temperature range. Used for one- and two-component adhesives, both solvent- or water-based. | |||||||||
Branched and linear Saturated Polyesters manufactured with synthetic acids and glycols.
Excellent mechanical properties and low density.
Branched and linear Saturated Polyesters manufactured with dicarboxylic acids and glycols.
Used in polyols for the production of sandals with low moulding density.
Being slightly branched, extraction time is reduced.
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 7025 B | Aliphatic | DEG | Branched | Liquid | 59 - 63 | 0,9 - 1,5 | 8800 - 9800 (35°C) | ≤ 0,1 | ≤ 150 |
| 7020 B | Aliphatic | DEG | Branched | Liquid | 64 - 68 | ≤ 0,5 | 4000 - 4600 (35°C) | ≤ 0,1 | ≤ 150 |
| FIELD OF USEMainly used for prepolymers and polyols for the production of women’s and men’s shoe soles with good performance in temperate climates. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 2030 A | Aliphatic | MEG, DEG | Linear | Waxy | 35 - 39 | ≤ 0,5 | 9000 - 10500 (35°C) | ≤ 0,1 | ≤ 100 |
| 2130 A | Aliphatic | MEG, DEG | Linear | Waxy | 38 - 42 | ≤ 0,1 | 8300 - 9300 (35°C) | ≤ 0,1 | ≤ 150 |
| 2020 B | Aliphatic | MEG, DEG | Linear | Waxy | 54 - 58 | ≤ 0,5 | 4200 - 4700 (35°C) | ≤ 0,1 | ≤ 100 |
| 2010 B | Aliphatic | MEG, DEG | Linear | Waxy | 108 - 116 | ≤ 0,5 | 1150 - 1250 (35°C) | ≤ 0,1 | ≤ 100 |
| FIELD OF USECan be used for the production of prepolymers and polyols. Good flexing resistance and physical properties. Used in the production of men’s and women’s footwear in temperate climates. | |||||||||
| ELAPOL | ACIDS/ ANHYDRIDES | MAIN GLYCOLS | STRUCTURE | APPEARANCE | OH NUMBER | ACID NUMBER | BROOKFIELD VISCOSITY | WATER CONTENT | HAZEN COLOUR |
|---|---|---|---|---|---|---|---|---|---|
| mg KOH/g | mg KOH/g | mPa·s | % | ||||||
| 1120 B | Dicarboxylic | MEG, DEG | Linear | Liquid | 54 - 58 | ≤ 1 | 700 - 850 (75°C) | ≤ 0,1 | ≤ 12 (Gardner) |
| 1020 A | Dicarboxylic | MEG | Branched | Liquid | 60 - 64 | ≤ 1 | 9000 - 11000 (35°C) | ≤ 0,03 | ≤ 12 (Gardner) |
| 1030 B | Dicarboxylic | MEG | Branched | Liquid | 36 - 40 | ≤ 1 | 5000 - 6000 (50°C) | ≤ 0,1 | ≤ 10 (Gardner) |
| FIELD OF USEUsed in polyols for the production of sandals with low moulding density. Being slightly branched, extraction time is reduced. | |||||||||